Gear Failure Analysis: Reading Fracture and Flank Damage Back to Root Cause

A photo of a failed gear arrives with one question attached: why did it break. Before answering, keep the part intact. Do not wash the fracture, do no

A photo of a failed gear arrives with one question attached: why did it break. Before answering, keep the part intact. Do not wash the fracture, do not grind it, do not fit the two halves back together, do not tap it with a hammer. Photograph it in place, then record running hours, load profile, lubricant grade and oil-change history. The most expensive mistake in failure analysis is not a wrong conclusion; it is destroyed evidence.

Start by separating tooth breakage from surface damage. A tooth that broke out at the root fillet, with beach marks running across the fracture and a rough final zone, failed in bending fatigue. A fracture with a fresh, bright surface, plastic deformation or a tooth top beaten flat points first at impact load or a foreign object passing through the mesh. One root broken while the loaded flank is polished and dented usually means overload, not fatigue. On the flanks, position is the first clue. Pitting that begins near the pitch line is contact fatigue. Pitting that starts at the tip or the root suggests the contact pattern has been pushed to the edge by a profile error, or that lubrication is starved or running too hot.

Four surface damage modes, four different signatures. Pitting starts as small craters, spreads in patches and eventually links into spalling. A spall has a flat floor and a steep edge, and it exposes material softer than the case; that points to a case that is too shallow or a core that is too soft. Scuffing pulls grooves along the sliding direction, with material transfer and welded traces, and it happens where the oil film breaks down at high speed and load — the contributors are flank roughness, the extreme-pressure performance of the oil, and oil supply during start-up. Abrasive wear thins the flank evenly, sharpens the tip and grows the backlash; the source is usually foreign particles, so check filtration and assembly cleanliness. Plastic deformation shows as flanks squeezed down and tips rolled over, and it follows either insufficient surface hardness or a short period of severe overload.

Hardness and case depth are the coordinates you cannot skip. For carburized and quenched parts in 20CrMnTi, the usual targets are 58 to 63 HRC at the surface, 30 to 42 HRC in the core, and an effective case depth of 0.5 to 2.0 mm. A soft core lets the root deflect, and spalling of the case follows. Quenched and tempered 42CrMo runs at 269 to 321 HB; only at that level is pitting life worth discussing. Induction-hardened parts sit at 48 to 58 HRC with a hardened depth of 1.0 to 5.0 mm. Nitrided parts reach 850 HV and above with a layer of 0.3 to 0.6 mm. When measured values miss the drawing, read the heat-treatment records and the position of the part in the furnace before redesigning anything. Case depth is measured to GB/T 9450 or ISO 2639; martensite grade and retained austenite are rated to GB/T 25744. High retained austenite keeps transforming in service, and dimensions and tooth form drift with it.

Geometry that is not held shortens life just as surely. A profile slope error, positive or negative, pushes the contact pattern off the middle of the flank toward the tip or the root, raises local stress, and pitting starts there. A lead slope error loads one end of the face width while the other end barely participates, so fatigue appears first at the loaded edge. Radial runout brings eccentricity, backlash opens and closes once per revolution, and impact loading rises with it. If the pre-grind allowance is too small, heat-treatment distortion cannot be absorbed, the flank keeps part of its decarburized skin or is ground unevenly, and early failure is close to certain.

Grinding burn does not show itself to the eye. A bright flank with temper colour neither proves nor excludes burn. Confirm it by acid etch or microstructural examination; where a re-tempered layer exists, the part is rejected or reworked. Burn tends to appear in clusters within a batch, which points at a stable deviation in wheel dressing, infeed or coolant, not at one bad piece. Check the process window, not a single part.

Prevention sits in three places. Keep a test coupon from the same heat as the production batch, so a failure can be traced back to a furnace load and a process curve. Set pre-grind allowance from the module and from measured distortion, not from a single rule of thumb. Put hardness, case depth, accuracy grade and the measurement datum on the shipping documents, so the assembly floor can compare instead of guessing. Two things on the user side matter as much: running within the design load, and changing oil and checking filtration on schedule. Most scuffing and abrasive wear failures start in those two places.

One industry note. Gear Technology’s State of the Gear Industry 2026 survey, published 4 March 2026 with 137 respondents, reports that when new equipment is expensive or hard to source, users keep existing machines running longer, which keeps overhaul and repair work busy. In the same survey, customers are pushing noise specifications tighter, with “noiseless gears” now rippling back through design, cutting and finishing (source: Gear Technology, 4 March 2026, https://www.geartechnology.com/state-of-the-gear-industry-2026). For buyers this means replacement gears are increasingly reverse-engineered from the worn part. Miss any one of three items — material grade, heat-treatment process, accuracy grade — and the replacement fails the same way the original did.

If you have a failed part, or a gear to be reproduced from a worn sample, send the fracture photos, the original drawing or measured dimensions, material and hardness data, and quantity to www.geyontech.com. We answer per part with the process route we would run, the accuracy grade we can hold and the inspection items we would report.

Send us a drawing — get engineering feedback first

Upload a 2D/3D drawing (STEP, DXF, PDF) — we reply with a quote and lead time.