A drawing arrives with “20CrMnTi or equivalent” in the material box and one question attached: can you make it. Yes — but three things have to be sett
A drawing arrives with “20CrMnTi or equivalent” in the material box and one question attached: can you make it. Yes — but three things have to be settled first. What kind of load the tooth actually sees, how large the section is, and whether the flanks will be ground after heat treatment. Leave those open and the same drawing supports three different steels, three process routes and three prices.
Load type comes first. Where contact fatigue dominates — pitting, then spalling — the part needs high surface hardness and enough case depth to carry it. Where bending fatigue at the root dominates, it needs core toughness and a generous root fillet. When both are present, the job belongs to a carburizing steel. On parts that take impact, more surface hardness buys very little; more core hardness and impact energy buys a lot. Carburized 20CrMnTi settles at 30 to 42 HRC in the core with Rm of 1080 MPa and above and Akv of 55 J and above. That combination was designed for small and medium module gearbox gears that see shock, and it still fits them.
Section size decides whether a grade can do the job at all. Hardenability sets the section a given grade can harden through. 20CrMnTi suits small and medium modules. Scale the section up and the core stays soft, the root deflects further under load, and the case spalls off behind it. For heavy sections, quenched and tempered 42CrMo at 269 to 321 HB, with Rm of 1080 MPa and above, ReL of 930 MPa and above and Akv of 63 J and above, is the more defensible answer; so is carburized 20CrNi2Mo with a 28 to 42 HRC core and 0.8 to 3.0 mm of effective case. Buying steel is not about picking the better grade. It is about picking the one that actually hardens at your section.
The heat-treatment route is the third gate. Carburizing runs at 920 to 940 °C, quenches at 820 to 850 °C, tempers at 180 to 200 °C: 58 to 63 HRC at the surface, 0.5 to 2.0 mm of effective case, visible distortion, a generous pre-grind allowance, and grinding as a fixed step in the route. Quench and temper at 840 to 860 °C with tempering between 540 and 620 °C gives 269 to 321 HB with little distortion, so most parts only need finish turning before assembly. Nitriding at 500 to 530 °C for 20 to 60 hours produces 0.3 to 0.6 mm at 850 HV and above with almost no dimensional change, which makes it a natural last step after grinding. Settle the route before you fix the tolerance block, and the accuracy grade on the drawing has a chance of holding.
Grade cross-references are for communication, not for substitution. 42CrMo is 42CrMo4, 1.7225, SCM440, AISI 4140. 40Cr is 41Cr4, SCr440, AISI 5140. 45 steel is C45, S45C, AISI 1045. 20CrMo is 20CrMo5, SCM420, AISI 4118. 20CrNiMo is 20NiCrMo2-2, SNCM220, AISI 8620. 38CrMoAl is 31CrMoV9, SACM645. 20CrMnTi is a GB/T 3077 grade with no one-to-one counterpart in DIN or AISI, so substituting it means checking carbon and alloy ranges plus the end-quench curve. A similar name is not evidence.
“Equivalent” usually fails in three places. Hardenability is the first: two heats carrying the same name can separate along the Jominy curve, and a large section feels that separation long before a small one does. Cleanliness and structure come second: grain size 5 to 8, non-metallic inclusions A ≤ 2.5, B ≤ 2.5, C ≤ 2.0, D ≤ 2.0, general porosity ≤ grade 2. Leave those out of the purchase specification and you receive whatever the mill runs on a normal day. Heat treatment is third. Change the steel and the carburizing temperature, carbon potential, quench medium and tempering temperature all have to be set again. Reusing the old curve on a new grade is a bet, and it usually loses on the first batch, in the form of distortion the grinder cannot absorb or a case that comes out shallow at one end of the load.
Incoming inspection is done per heat, not per impression. Spectrometry on one piece per heat for chemistry. Tensile testing plus hardness on two pieces per lot for mechanical properties. Acid etch on one piece per heat for porosity. Dimensions and appearance at AQL 1.0, Level II. The records stay in the batch file. When a customer asks two years later what went into a part, a document answers and a memory does not.
How we quote material. By default we quote Chinese equivalent grades: 17CrNiMo6 in place of 18CrNiMo7-6 (1.6587), 42CrMo in place of 42CrMo4. Both pairs have run in gear work long enough that the properties line up with what drawings ask. When a drawing names a European grade together with a mill-origin requirement, we put the substitution and its differences in writing and wait for the customer’s written confirmation before quoting price and lead time. Material substitution is not a decision a supplier makes on its own.
One industry note. China’s State Administration for Market Regulation, through Announcement No. 43 of 2026, released two harmonic-drive standards: GB/T 12601-2026, Basic terminology of the harmonic gear drive, and GB/T 14118-2026, Harmonic drive reducers. Both were published on 28 September 2026, take effect on 1 April 2027, and fully replace the 1990 and 1993 versions respectively. The drafter list includes Suzhou Leaderdrive, Zhejiang Laifual Harmonic Drive and Ningbo Zhongda Leader (source: National Standards Information Public Service Platform, https://std.samr.gov.cn/gb/search/gbDetailed?id=5CB12E0EFB662034E06397BE0A0A34FB). For buyers of robot joint components, this is the first revision in more than three decades, which means terminology and test items now have a common reference. A drawing marked for harmonic reducer use needs its material and heat-treatment requirements checked against the new text before it goes out for quotation.
If you are choosing a steel, or holding a drawing that says “or equivalent” and want to know whether the substitution holds, send the drawing, the load case, the material and heat treatment used before, and the quantity to www.geyontech.com. We answer per part with the grade we would run, the route behind it, and the inspection we would report.